Chemical composition
WC (including doping): 88,0%
Co: 12,0%
Physical Characteristics
Density: 14,12 g/cm³ ± 0,1
Hardness: 92,5 HRA ± 0,3
Coercitive Force: 310 Oe ± 50
Magnetic Saturation: 140-162 G*cm³/g
TRS: 4500 N/mm2
Structure
Grain Size: 0,4 μm
Porosity: <A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations
Chemical composition
WC (including doping): 91,5 %
Co: 8,5 %
Physical Characteristics
Density: 14,55 g/cm3 ± 0,1
Hardness: 93,8 HRA ± 0,3
Coercitive Force: 380 Oe ± 50
Magnetic Saturation: 140-162 G*cm³/g
TRS: 4700 N/mm2
Structure
Grain Size: 0,4 μm
Porosity: <A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations
Chemical composition
WC (including doping): 91,0%
Co: 9,0%
Physical Characteristics
Density: 14,58 g/cm³ ± 0,1
Hardness: 91,0 HRA ± 0,3
Coercitive Force: 180 Oe ± 30
Magnetic Saturation: 140-162 G*cm³/g
TRS: 3200 N/mm2
Structure
Grain Size: 2,0 μm
Porosity: <A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations
General Characteristics
Suitable for stainless steel manufacturing, nickel-based alloy (super alloys), titanium alloys. Suitable for roughing drilling of irregular surfaces of stainless tender or tough. It is not appropriate to process hardened steel.
Chemical composition
WC (including doping): 88,0%
Co: 12,0%
Physical Characteristics
Density: 14,22 g/cm³ ± 0,1
Hardness: 91,1 HRA ± 0,3
Coercitive Force: 210 Oe ± 30
Magnetic Saturation: 140-162 G*cm³/g
TRS: 3740 N/mm2
Structure
Grain Size: 0,8 μm
Porosity: <A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations
Chemical composition
WC (including doping): 90,0%
Co: 10,0%
Physical Characteristics
Density: 14,42 g/cm³ ± 0,1
Hardness: 92,1 HRA ± 0,3
Coercitive Force: 230 Oe ± 30
Magnetic Saturation: 140-162 G*cm³/g
TRS: 3700 N/mm2
Structure
Grain Size: 0,8 μm
Porosity: <A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations
Chemical composition
WC (including doping): 94,0%
Co: 6,0%
Physical Characteristics
Density: 14,80 g/cm³ ± 0,1
Hardness: 93,4 HRA ± 0,3
Coercitive Force: 300 Oe ±
Magnetic Saturation: 150 G*cm³/g
TRS: 2600 N/mm2
Structure
Grain Size: 0,8 μm
Porosity: A00; B00; C00
Metallographic Analysis: Free of eta – phase and contaminations